Ask Lasest Price | |
Brand Name : | ramimtech |
Certification : | ISO |
Price : | 1 |
Delivery Time : | 5 days |
Payment Terms : | TT |
Supply Ability : | 10000rolls/month |
Conveyor belt repair strip instruction for use
Image1. Choosing one piece of conveyor belt repair stirp which is 2-3mm larger than damage area. As damage area is center,
drawing out marking line.
Making preparation work for roughening.
1.Choosing one piece of repair stirp which is 2-3mm larger than
damage area.As damage area is center, drawing out marking line.
Making preparation work for roughening.
Images2. Roughening damage area by using of angle grinder which is
with high power and low speed and is equiped with tungsten steel
grinding disc.
2.When roughening damage area,we recommend angle grinder
RAMIMTECH-L1202 which is with high power and low speed and is
equiped with tungsten steel grinding disc.
the value of roughening depth can't be smaller than the thickness
value of repair stirp. For instance, the thickest part of 150mm
fabric reinforced repair stirp is 4.6mm, so we need roughen 4.6mm
to avoid repair strip being scraped by belt cleaner.
Image3. Using non-flammable cleaning solution to clean roughened
area.
3.Clean the roughened area by using cleaning solution SK353 and
then wait it dry.
Image4. Pouring hardener UT R40 into cold vulcanizing glue ,and
stiring it well at the same time.
4.While waiting cleaning soluiton dry, we can mix cold vulcanizing
glue with hardener UT R40 and make two components mix well.
Image5. Brushing the mixture of cold vulcanzing glue SK313 and UT
R40 to the whole surface which need repair, and waiting it dry to
the degree that do not stick finger back.
5.Brushing the mixture of cold vulcanzing glue SK313 and UT R40 to
the whole surface which need repair, and waiting it dry to the
degree that do not stick finger back.Be sure to brush evenly at the
same thickness on the whole surface.
Image6. Brushing mixture of cold vulcanizing glue SK313 and UT R40
onto the blue bonding layer of repair strip and wait it dry to the
degree that it is slightly stick.
6.Brushing mixture of cold vulcanizing glue SK313 and UT R40 onto
the blue bonding layer of repair strip and wait it dry to the
degree that it is slightly stick.
Image7. When bonding RIT conveyor belt cold vulcanizing repair strip onto belt,use roller stitcher to roll the surface firmly.
7.When bonding RIT repair strip onto belt,use roller stitcher to
roll the surface firmly.
Image8.After bonding,need brush one coat mixture glue at the
bonding edge of repair strip and conveyor belt , and make the edged
CN layer of repair strip have cold vulcanizing reaction by itself.
8.After bonding,need brush one coat mixture glue at the bonding
edge of repair strip and conveyor belt , and make the edged CN
layer of repair strip have cold vulcanizing reaction by itself.
Image9. If damage need a few of repair strips, look out the lap
way. we can operate as image showed.
9.If damage need a few of repair strips, look out the lap way. we
can operate as image showed.
Special operation pionits of conveyor belt repair strip.
1.Ramimtech materials must be stored at cool dry ventilated place.
2.Temperation of loading material on conveyor belt under 90 ℃.
3.Please use repair materials with non-flammble lable when do
underground repair.
4.Bond repair stirp and repair patch in embedded way to avoid of
being scraped by belt cleaner.
5.If the surface for bonding is damp,must make it dry before
bonding.
6.Do not burn the surface when roughening,abrasion wheel is not
allowed to use,only can use RIT tungsten carbide buffing disc.
7.Use steel brush to clear off dust and rubber scraps,and use
RAMIMTECH cleaning solution to clean the surface.
8.Glue mixture:when do seamless jointing and repair of belt
,Ramimtech cold vulcanizing glue Sk313 need to be mixed with
hardener by the ratio of 100:4, and be stired evenly.
9.Ramimtech mixtrue must be brushed by mane brush hard and evenly
to make SK313 mixture can be infiltrated into rubber surface.
Belt surface need brush two coats Sk313 mixture while the blue CN
layer of repair strip be brushed one coat.
All the coats need keep from dust and damp.
10.The drying time of cold vulcanizing glue SK313 mixture depend on
air temperature, humidity and absorbent of conveyor belt itself.
The first coat on belt need dry to degree of do not stick finger
back and the second to the degree of slightly stick.
While brushing the second coat on belt ,need brush one coat onto CN
bonding layer of repair strip at the same time.
11.Ensure both bonding surface are dry and clean.
12.Rolling must be started from center to edge. when the first
rolling fix position of repair strip, roll second time to extrude
air and make bonding firm.
![]() |